Understanding Galvanostatic Charge–Discharge Curves: Voltage Plateaus, Slopes, and Linear Regions

discharge curves at different rates at room temperature

What Do Charge–Discharge Curve Shapes Reveal About Battery Thermodynamics, Energy Storage Mechanisms, and Electrochemical Performance?

Galvanostatic charge–discharge (GCD) curves are widely used to characterize lithium-ion batteries, sodium-ion batteries, supercapacitors, and other electrochemical energy storage devices.

At first glance, these curves may appear simple: voltage rises during charging and falls during discharging.

However, their shapes contain valuable information about electrode thermodynamics, ion storage mechanisms, electrochemical kinetics, internal resistance, and energy storage behavior.

Why do some batteries exhibit flat voltage plateaus while others show continuous slopes?

Why do supercapacitors often produce nearly triangular charge–discharge curves?

And why can the same electrode material display different voltage profiles when the current changes?

Understanding these differences is essential for interpreting electrochemical test results correctly.

1. What Do Voltage Plateaus, Slopes, and Linear Regions Represent?

During a galvanostatic charge–discharge test, the instrument maintains a specified current while recording voltage as a function of time.

The current direction reverses between charging and discharging, while voltage generally increases or decreases according to the device’s state of charge.

The vertical axis may represent either:

  • Full-cell voltage: The potential difference between the positive and negative electrodes.
  • Single-electrode potential: The potential of an electrode measured relative to a reference electrode.

The horizontal axis typically represents time or transferred charge.

For a constant-current segment:

Q = |I| × Δt

Where:

  • Q: Transferred charge (Ah)
  • I: Current (A)
  • Δt: Time (h)

Dividing transferred charge by the mass of active material gives the specific capacity, typically expressed in mAh/g.

Time and transferred charge are proportional within a constant-current segment. However, when the current changes, the amount of charge transferred during the same time interval also changes.

What Is a Voltage Plateau?

A voltage plateau is a region where substantial charge is transferred while the voltage changes only slightly.

What Is a Sloping Region?

A sloping region is a section where voltage changes continuously as charge is transferred.

Its slope may remain approximately constant or vary throughout the process.

What Is a Nearly Linear Region?

A nearly linear region has an approximately constant slope and relatively small curvature.

These descriptions are not mutually exclusive.

A tilted straight line is also a slope, while an almost horizontal line can be described as a plateau.

A more useful parameter is the local slope:

dV/dQ

Where V is voltage and Q is cumulative transferred charge.

  • dV/dQ ≈ 0: Nearly flat voltage plateau
  • Approximately constant, nonzero dV/dQ: Nearly linear voltage region
  • Changing dV/dQ: Curved voltage profile

The key question is not whether current continues flowing.

It is how much the voltage changes for each additional unit of transferred charge.

Article content

Research reference: DOI: 10.1038/s43588-021-00153-5

This study examines electrode structures, ionic liquid models, and galvanostatic charging behavior in supercapacitor systems.


2. Why Does Voltage Change as Charge Is Stored?

The voltage response of an electrochemical system is closely related to its thermodynamic properties.

Battery electrodes store charge through processes such as ion insertion, extraction, and electrochemical conversion.

Near equilibrium, electrode potential is related to the chemical potential of the active species.

Under constant temperature and pressure, chemical potential can be expressed through the derivative of Gibbs free energy with respect to the amount of a component, under the appropriate thermodynamic constraints.

This relationship helps explain why some electrode materials exhibit flat voltage plateaus while others produce continuous slopes.

Why Does Voltage Remain Nearly Constant During Two-Phase Reactions?

Consider an electrode material in which two phases with different compositions coexist.

During charging or discharging, additional ion insertion or extraction may primarily change the relative proportions of the two phases.

The compositions of the individual phases remain within relatively narrow ranges.

Under ideal two-phase equilibrium conditions, the common-tangent construction of the free-energy curve gives the same chemical potential for the coexisting phases.

As the overall composition changes within the two-phase region, the chemical potential remains approximately constant.

The corresponding electrode potential therefore forms a voltage plateau.

In other words:

Charge continues to transfer, but the equilibrium voltage changes very little because the relative amounts of the two phases are changing.

Research on P2-type sodium layered oxides has compared voltage plateaus derived from free-energy fitting with relaxed electrode potentials obtained through intermittent titration.

The two-phase coexistence region corresponds to changes in phase proportions, while the single-phase regions near its boundaries retain continuous voltage slopes.

Article content
Free energy fitting of sodium layered oxides, two-phase coexistence regions and equilibrium voltage, and comparison with relaxation potentials from intermittent titration

Research reference: DOI: 10.1038/s41524-024-01258-x

Does Every Voltage Plateau Indicate a Two-Phase Reaction?

Not necessarily.

Real electrodes differ from ideal thermodynamic models.

Several factors can modify an otherwise flat plateau:

  • Finite particle size
  • Mechanical stress
  • Nonuniform reaction rates among particles
  • Electrochemical polarization
  • Concentration gradients

These effects can make a plateau appear tilted or broadened.

Furthermore, a relatively flat voltage region does not independently prove that a two-phase reaction is occurring.

Side reactions may also consume charge within a narrow potential range.

Structural characterization, such as X-ray diffraction, is often required to establish whether a phase transformation actually occurs.

Why Do Single-Phase Solid-Solution Reactions Produce Sloping Curves?

In a single-phase solid-solution reaction, ions are inserted into or extracted from the same crystal phase.

Rather than primarily changing the proportions of two phases, the process continuously changes ion occupancy within one phase.

As composition changes, several factors may evolve:

  • Ion-site occupancy
  • Interactions between inserted ions
  • Transition-metal oxidation states
  • Local crystal structure
  • Chemical potential

Consequently, electrode potential changes continuously with composition, producing a sloping voltage profile.

Ordering transitions or entry into a two-phase region may introduce inflection points or short plateaus.

A representative example is the sodium-ion electrode material:

Na₂₋ₓFe₂(SO₄)₃

This material exhibits a continuous sloping charge–discharge profile.

Research combining electrochemical measurements, X-ray diffraction, and Mössbauer spectroscopy supports the interpretation of a single-phase reaction mechanism.

Article content
Continuous sloping charge-discharge curves of Na₂₋ₓFe₂(SO₄)₃, as well as discharge curves and capacity retention at different rates.

Research reference: DOI: 10.1038/ncomms5358

The important distinction is that the electrochemical curve records changes in potential, while structural measurements help identify the underlying material transformation.


3. Why Does a Nearly Linear Charge–Discharge Curve Not Necessarily Mean Pure Double-Layer Capacitance?

Supercapacitors often exhibit nearly triangular galvanostatic charge–discharge curves.

This behavior is commonly associated with capacitive energy storage.

However, a nearly linear voltage–time relationship does not necessarily mean that energy is stored exclusively through an electrical double layer.

The Relationship Between Current, Voltage, and Capacitance

For a near-quasi-static charging process without significant leakage or side reactions, differential capacitance is defined as:

Cdiff = dq/dV

Where:

  • Cdiff: Differential capacitance (F)
  • q: Stored charge (C)
  • V: Voltage (V)

Under constant-current conditions:

dV/dt = I/Cdiff

If capacitance remains approximately constant throughout the voltage range, voltage changes nearly linearly with time.

Reversing the current produces a corresponding descending segment.

This explains why an ideal capacitive system can generate a triangular charge–discharge profile.

Electrical Double-Layer Capacitance

Electrical double-layer capacitors store energy through charge separation and changes in ion distribution near the electrode–electrolyte interface.

When capacitance varies only slightly with voltage, the resulting GCD curve may approach a triangular shape.

Pseudocapacitance Can Produce Similar Curves

Pseudocapacitive systems store charge through fast, reversible Faradaic processes.

Unlike conventional battery reactions characterized by extended voltage plateaus, pseudocapacitive charge storage can occur over a broad potential range.

Consequently, pseudocapacitive materials may also exhibit nearly triangular charge–discharge profiles.

If capacitance changes with voltage or ion transport becomes limited, both double-layer and pseudocapacitive systems may show curved profiles.

Example: Porous MoN Single Crystals

Research on porous molybdenum nitride (MoN) single crystals demonstrated nearly triangular galvanostatic charge–discharge behavior in alkaline electrolyte.

However, the charge-storage mechanism was associated with surface OH⁻ chemisorption accompanied by changes in molybdenum oxidation state.

Spectroscopic characterization and computational analysis were used to investigate the active sites and underlying mechanism.

The charging curves also exhibited some curvature, indicating that the system did not behave as an ideal constant-capacitance device.

Article content
Cyclic voltammetry, near-triangular galvanostatic charge-discharge, impedance, cycling stability, and rate response of porous MoN single crystals.

Research reference: DOI: 10.1038/s41467-019-12818-x

This example highlights an important principle:

A nearly triangular charge–discharge curve is not sufficient evidence to distinguish pure electrical double-layer storage from reversible Faradaic pseudocapacitance.

Additional electrochemical and structural characterization is required.


4. How Do Current, Electrode Configuration, and Test Programs Change the Curve?

The shape of a measured charge–discharge curve is not determined by electrode thermodynamics alone.

Applied current, internal resistance, reaction kinetics, electrode configuration, and instrument control programs can all influence the observed voltage response.

Why Is the Voltage Under Current Different From the Relaxed Potential?

At finite current, measured voltage generally deviates from its equilibrium value.

The deviation includes contributions from:

  • Ohmic voltage drop
  • Charge-transfer polarization
  • Concentration polarization
  • Mass-transport limitations

During charging, the terminal voltage is generally higher than the corresponding equilibrium voltage.

During discharging, the terminal voltage is generally lower.

As current increases, these differences often become more pronounced.

Consequently, the same electrode material can exhibit different charge–discharge profiles at different current rates.

A flat equilibrium plateau may appear sloped during high-current operation.

Inflection points may become less distinct, and the accessible capacity may decrease.

What Does GITT Reveal?

The Galvanostatic Intermittent Titration Technique (GITT) alternates current pulses with relaxation periods.

During a current pulse, the measured voltage includes both thermodynamic and kinetic contributions.

When the current is interrupted, the voltage undergoes relaxation.

This response may include:

  • A relatively rapid voltage change associated with the removal of current-dependent contributions
  • Slower relaxation associated with concentration redistribution and other electrochemical processes

After sufficient relaxation, the measured potential may approach the equilibrium potential.

Research on P2-type sodium layered oxides has shown that the difference between operating voltage and relaxed potential changes with sodium content.

Some composition ranges exhibit greater polarization than others.

Article content
Current pulse and voltage relaxation of sodium layered oxides, comparison of potentials under load and at rest, and apparent diffusion coefficient.

Research reference: DOI: 10.1038/s41524-024-01258-x

These observations demonstrate that a measured voltage slope may contain both equilibrium thermodynamic behavior and kinetic effects.

Importantly, increasing the current and observing a more tilted plateau does not necessarily mean that the original two-phase region has disappeared.

Similarly, a finite relaxation period does not always establish true equilibrium.

Slow phase transformations, side reactions, and path-dependent hysteresis can cause charging and discharging potentials to remain different.

Why Can Full-Cell Curves Differ From Individual Electrode Curves?

A full-cell voltage represents the difference between the positive and negative electrode potentials.

Using a common reference:

Vcell = Epositive − Enegative

Both electrode potentials contribute to the full-cell voltage profile.

Therefore, even if one electrode exhibits a flat plateau, the full cell may still show a sloping voltage curve if the other electrode potential changes continuously.

This is particularly important when comparing half-cell measurements with commercial battery performance.

A voltage plateau observed in a single-electrode experiment cannot automatically be treated as the voltage plateau of the complete battery.

Why Is a Constant-Voltage Charging Segment Different From a Material Voltage Plateau?

Many lithium-ion batteries are charged using a constant-current/constant-voltage (CC–CV) procedure.

During the CC stage, current is held approximately constant while voltage rises.

Once the upper voltage limit is reached, the charger switches to the CV stage.

During the CV stage, the charger maintains a specified voltage while current generally decreases.

The resulting horizontal segment on a voltage–time graph is therefore created by the charging control program.

It does not necessarily represent a thermodynamic voltage plateau associated with a phase transition.

Because current changes during the CV stage, transferred charge must be calculated by integration:

Q = ∫ |I(t)| dt

It is incorrect to calculate the entire CV-stage capacity by multiplying a single fixed current by the elapsed time.

How Do Current and Cutoff Voltage Affect Capacity and Energy?

Higher current often produces greater polarization.

During discharge, increased polarization can cause the battery to reach its lower cutoff voltage earlier.

As a result, the test may end before all potentially accessible charge has been extracted.

Measured capacity therefore depends on operating conditions, including:

  • Applied current
  • Temperature
  • Upper and lower cutoff voltages
  • Relaxation conditions
  • Electrochemical kinetics

Capacity is determined by transferred charge.

Discharge energy, however, depends on both charge and voltage:

E = ∫ V dQ

A flat voltage plateau and a continuously sloping region can both contribute useful discharge energy.

Two batteries with the same measured capacity may deliver different amounts of energy if their voltage profiles differ.

This distinction is particularly relevant to practical battery applications where usable energy, rather than nominal capacity alone, determines operating performance.


Conclusion: Curve Shape Is a Starting Point, Not a Complete Mechanism

Galvanostatic charge–discharge curves provide important information about electrochemical energy storage systems.

However, their shapes must be interpreted carefully.

Voltage plateaus may reflect two-phase coexistence and relatively stable chemical potential.

Sloping regions may reflect continuous changes in chemical potential during single-phase solid-solution reactions.

Nearly linear regions may arise from approximately constant differential capacitance, including both double-layer and pseudocapacitive contributions.

Meanwhile, applied current, polarization, electrode configuration, relaxation behavior, and charging control programs can significantly alter the measured voltage profile.

The key principle is:

A charge–discharge curve shows how voltage responds to transferred charge under specific test conditions. It does not, by itself, uniquely identify the underlying energy storage mechanism.

Reliable interpretation requires combining electrochemical measurements with appropriate structural, spectroscopic, and kinetic analysis.

For practical battery engineering, understanding these relationships also helps explain why measured capacity, operating voltage, and usable energy can change with discharge rate, temperature, and cutoff conditions.


Research References

  1. Nature Computational Science — DOI: 10.1038/s43588-021-00153-5
  2. npj Computational Materials — DOI: 10.1038/s41524-024-01258-x
  3. Nature Communications — DOI: 10.1038/ncomms5358
  4. Nature Communications — DOI: 10.1038/s41467-019-12818-x